Skip to content
Skills / Apartment Maintenance / Apartment Maintenance Technician / Patching Concrete Cracks and Spalls
Apartment Maintenance

Patching Concrete Cracks and Spalls

20 min read Training Guide

Tell a harmless crack from one that needs an engineer, seal cracks with the right material, and patch spalled sidewalks, steps and slabs with square cuts, a good bond and proper curing.

Table of contents

Sidewalks, steps, curbs, patios and garage floors crack and chip. Water gets in, freezes, and pops off more. Rust swells the steel inside and breaks off the surface over it. Left alone, a small spall grows into a trip hazard and a liability. Most of these repairs are routine work for maintenance and handyman crews. A few are signs of a structural problem that no patch should hide, and the first skill is telling the two apart.

The repair steps in this guide follow the American Concrete Institute's repair bulletin for surface repairs and the general practice in its crack repair guide. The repair product's instructions control the details, such as thickness, mixing, temperature and curing, so read the bag or the data sheet before you start.

What You Will Be Able to Do

  • Tell a surface defect you can repair from a structural problem that needs an engineer.
  • Find the cause of a crack or spall before you fix it.
  • Choose a sealant or repair material for a crack, a spall or a trip hazard.
  • Prepare, bond, place and cure a spall repair that stays put.
  • Control silica dust and protect yourself from wet cement.

Terms

  • Crack: a break through the concrete. Hairline cracks are very thin. Wider cracks may be moving.
  • Dormant crack: a crack that is not moving or growing.
  • Active crack: a crack that opens and closes with temperature, moisture or loads, or keeps growing.
  • Spall: a piece of the surface that has broken off, leaving a pit.
  • Scaling: thin flakes peeling off the top surface, often from freezing and deicing salts.
  • Delamination: a layer that has separated below the surface but has not fallen off yet. It sounds hollow when tapped.
  • Feather edge: a patch that thins out to nothing at its edges. Feather edges break off.
  • SSD (saturated surface dry): concrete that has soaked up water but has no standing water or shine on top.

When to Stop and Call an Engineer

Stop and report it, without patching, when you see any of these:

  • Cracks in foundation walls, beams, columns, retaining walls, balconies, or parking garage decks.
  • Cracks wider at one end, cracks with one side higher than the other, or cracks that keep growing.
  • Doors and windows nearby that have started to stick, or floors that have sunk or tilted.
  • Rusted steel bars with noticeable loss of metal, or several bars exposed.
  • Concrete that is cracked through near anchors, railings or posts that hold people up.

The ACI repair bulletin says that when reinforcing steel has lost significant section, a structural engineer should decide the repair. A patch over a structural problem hides the warning sign and makes the real repair harder.

Find the Cause First

The ACI bulletin's first step is finding the root cause, or the repair will fail the same way.

Cause What you see Fix the cause
Freezing and thawing, deicing salts Scaling, pitting, crumbling edges Better drainage, sealer, change the deicer
Rusting steel inside Rust stains, spalls over a bar Remove concrete to clean steel, protect it
Settlement or poor base Cracks with one side lower, slabs tilting Fix the base or replace the slab
Tree roots Slabs lifted near trees Root work by a qualified arborist, or replacement
Water pooling or downspouts Damage where water collects Regrade, redirect downspouts
Impact Chipped edges, broken corners Protect the edge, such as a curb guard
Shrinkage Random hairline cracks soon after placing Usually harmless, seal if needed

Choosing the Repair

Problem Typical repair
Hairline dormant cracks Often left alone, or sealed with a penetrating crack sealer
Wider dormant cracks Crack filler or sealant rated for that width
Active cracks and joints Flexible sealant that can stretch, with backer rod where deep
Shallow spall or pothole Repair mortar patch, following this guide
Large area of scaling Resurfacer over a cleaned surface, or replacement
Deep or widespread damage Replace the section
Uneven sidewalk joint Grind, ramp or replace, depending on the height

Cracks

  • Active cracks need flexible material. Cement and rigid epoxy in a moving crack just crack again. Use a flexible sealant made for concrete. Self-leveling sealants flow into horizontal cracks and joints.
  • Make a reservoir. For a crack too thin to fill, routing or sawing a small groove along it gives the sealant enough room and depth to hold. Clean out the dust before sealing.
  • Backer rod goes into deeper cracks and joints so the sealant has the right depth and sticks only to the sides.
  • Epoxy injection glues a dormant crack back together. It is for trained crews working from an engineer's plan, not for sealing a moving crack.

Trip Hazards

Sidewalks along accessible routes follow the ADA Standards for changes in level. Those numbers are a good guide for any walkway.

Change in level ADA rule
Up to 1/4 inch Allowed as is
Over 1/4 inch up to 1/2 inch Bevel it, no steeper than 1 to 2
Over 1/2 inch Needs a ramp, or the slab must be ground, raised or replaced

Until a trip hazard is fixed, mark it and block it off, and report it.

Safety

Silica Dust

Sawing, grinding and chipping concrete throws crystalline silica dust, which causes permanent lung disease. OSHA's silica rule for construction, 29 CFR 1926.1153, gives approved methods in Table 1. Under those methods:

Tool Control Respirator outdoors Respirator indoors
Handheld saw Water at the blade None up to 4 hours, APF 10 over 4 hours APF 10
Jackhammer or chipping tool Water spray, or a shroud with a dust collector None up to 4 hours, APF 10 over 4 hours APF 10
Handheld grinder for surface work Water outdoors, or a shroud with a dust collector None None up to 4 hours, APF 10 over 4 hours, with the shroud

APF 10 means a respirator with an assigned protection factor of 10, such as a fitted half-mask with the right filters. The employer decides the respirator and runs the fit testing. Do not dry sweep the dust. Clean up wet or with a HEPA vacuum.

Wet Cement

Wet cement and repair mortar are strongly alkaline and can cause chemical burns, sometimes without much pain at first.

  • Wear waterproof gloves, long sleeves and eye protection when mixing and placing.
  • Do not kneel in wet mortar without waterproof knee pads.
  • Wash wet mortar off skin right away with clean water. If it gets in your eyes, flush them with water and get medical help.

Other Hazards

  • Noise and impact. Wear hearing protection and safety boots with chipping hammers and saws.
  • People nearby. Block off the work area with cones or barricades, and keep it blocked until the patch has cured.
  • Lifting. Bags of repair mortar are heavy. Lift with your legs and get help with buckets.

Patching a Spall

  1. Find all the damage. Tap the area around the spall with a hammer. Sound concrete rings. Delaminated concrete sounds dull or hollow. Mark the full area of hollow and broken concrete.
  2. Draw a simple shape. Outline the repair as a square or rectangle around the damage, extending into sound concrete. Avoid L-shapes and inside corners, which crack.
  3. Sawcut the edges. Cut straight down along the outline, about 1/2 inch deep, so the patch has a square shoulder instead of a feather edge. Do not cut into any steel bars. Use water at the blade.
  4. Remove the damaged concrete. Chip out everything inside the cuts down to sound, solid concrete. Use a light chipping hammer, not a heavy breaker, so you do not crack the good concrete underneath.
  5. Free any exposed steel. If rusted bars are exposed, chip about 3/4 inch behind them so the repair material can wrap all the way around. Clean off the loose rust. If a bar has lost much of its metal, stop and report it.
  6. Clean the surface. It should be rough, sound, and free of dust, oil and loose bits. Blow it off or vacuum it.
  7. Wet it if the product calls for it. For cement-based repair mortars, the ACI bulletin calls for the surface to be saturated surface dry: soak it, then remove standing water, so the old concrete does not suck the water out of the patch. Some products with a bonding agent must go on a dry surface instead. Follow the label.
  8. Apply a bond coat. Scrub a thin coat of the repair mortar, mixed without extra water, into the surface with a stiff brush. Or use the bonding agent the product calls for. Place the patch while the bond coat is still wet.
  9. Place the repair mortar. Mix it to the label, without extra water, which weakens it. Press it in firmly, working it into the edges and around any steel. Place deep repairs in layers within the product's thickness limits, and scratch each layer so the next one bonds.
  10. Finish to match. Strike it off level with the surrounding surface, then float and broom it to match the texture around it.
  11. Cure it. Keep the patch from drying out too fast, as the label directs, with a curing compound or by keeping it damp and covered. Protect it from freezing, hot sun, wind and traffic for the time the product lists.
  12. Check it. After it cures, tap the patch and its edges. A hollow sound means it did not bond.

Worked Example: Sizing a Sidewalk Patch

A spall on a sidewalk is about 10 inches by 12 inches, and tapping shows hollow concrete a couple of inches past its edges.

  • Outline: draw a rectangle around the hollow area, extending into sound concrete. Say it comes to 14 inches by 18 inches.
  • Depth: after chipping to sound concrete, the hole averages 1-1/2 inches deep.
  • Volume: 14 x 18 x 1.5 = 378 cubic inches. There are 1,728 cubic inches in a cubic foot, so 378 / 1,728 = 0.22 cubic feet.
  • Material: check the bag for its yield in cubic feet and its thickness limits. If 1-1/2 inches is within the limits for one layer and one bag yields more than 0.22 cubic feet, one bag does it, with a little extra for the bond coat.

Sealing a Dormant Crack

  1. Clean it. Remove dirt, loose concrete and old filler with a wire brush or a crack chaser, then vacuum or blow it out.
  2. Widen thin cracks with a grinder and crack-chasing wheel if the sealant needs more room, using a Table 1 dust control method.
  3. Add backer rod in deep cracks to set the sealant depth the product calls for.
  4. Fill it. Apply the sealant or filler, tool it smooth, and keep traffic off until it cures.

Common Mistakes

Mistake What happens
Patching without finding the cause The patch fails, or the damage moves next door
Feather edges Thin edges break off in weeks
Not removing all hollow concrete The patch pops off with the layer under it
Patching over dust or oil No bond
Adding extra water to the mix A weak, dusty, cracked patch
Rigid filler in a moving crack It cracks again
No curing Shrinkage cracks and a weak surface
Patching a structural crack The warning sign is hidden

Check Your Understanding

1. A sidewalk slab has heaved, and one side of a joint is 3/4 inch higher than the other. What does it need?

That is more than 1/2 inch, so under the ADA Standards it needs a ramp, or the slab must be ground down, raised or replaced. Mark and block it off until it is fixed.

2. You chip out a spall on a balcony and find two rusted bars that are noticeably thinner than they should be. What do you do?

Stop and report it. A balcony is structural, and steel that has lost section needs a structural engineer to decide the repair.

3. Why do you sawcut the edges of a spall repair instead of just filling the hole?

Sawcut edges give the patch a square shoulder at full thickness. Without them, the patch thins to a feather edge that breaks off.

4. A crack in a patio opens wider every winter and closes in summer. What should you fill it with?

It is an active crack, so use a flexible sealant made for concrete, with backer rod if it is deep. Rigid cement or epoxy would crack again.

Key Takeaways

  • Cracks in structural concrete, displaced slabs, and steel with section loss go to an engineer.
  • Find the cause first: water, freezing, rusting steel, settlement or roots.
  • Use flexible sealant in moving cracks, and patch spalls with square sawcut edges into sound concrete.
  • Bond, place and cure the repair exactly as the product label says, without extra water.
  • Control silica with a Table 1 method, and protect skin and eyes from wet cement.