Preparing a Substrate for Tile
Judge whether a floor or wall is stiff, sound and bondable enough for tile, choose between backer board and membranes, and install them so the tile above stays bonded.
Table of contents
The substrate is everything under the tile: the framing, the subfloor or slab, and any board or membrane on top. Tile cannot bend, so it takes on every flaw below it. A bouncy floor cracks grout lines. A sealed slab lets tiles pop loose. Wet drywall behind a shower crumbles. Most tile failures trace back to a substrate problem that was visible before the job started.
What You Will Be Able to Do
- Check a wood floor for stiffness and know when the fix belongs to a framer or engineer.
- Tell whether a slab will bond and whether its cracks can be covered.
- Choose cement board, fiber-cement board or a membrane for the job in front of you.
- Install backer board and membranes so they do what they are rated for.
- Name the surfaces tile should never go on directly.
What Tile Needs From Below
| Need | Why it matters | How you check |
|---|---|---|
| Stiff | Flex cracks tile and grout | Span math, bounce test, look at framing |
| Flat | Humps and dips cause lippage and hollow spots | Long straightedge, per the tile size rule |
| Sound and clean | Mortar bonds only to a clean, solid, open surface | Scrape, scratch, water drop test |
| Right for the area | Wet areas need materials that water does not damage | Read the product rating |
Flatness tolerances and how to fix a floor that is out of flat are their own job. Measure and correct flatness before you install the layers below.
Stiffness on Wood Floors
Deflection is how far a floor bends under load. The tile industry measures it as a fraction of the span, written L/360 or L/720, where L is the joist span in inches.
| Tile | Common deflection limit |
|---|---|
| Ceramic and porcelain | L/360 |
| Natural stone | L/720 |
Worked example. A floor's joists span 13 feet 6 inches, or 162 inches. At L/360, the floor may bend no more than 162 / 360 = 0.45 inch at the center under design load. For stone, at L/720, the limit is 162 / 720 = 0.225 inch. That is half as much, which is why stone needs much stiffer framing.
You cannot measure L/360 with a tape. It comes from the joist size, species, grade, spacing and span, checked against span tables or an engineer's numbers. On the job, look for the warning signs:
- The floor bounces or rattles dishes when you walk across it.
- Joists are notched, cut for pipes, or sagging.
- Old tile has cracks that run in a line across several tiles.
- Joists are spaced wider than 16 inches on center.
There are two kinds of flex. Joist deflection is the whole floor sagging between its supports. Subfloor deflection is the plywood flexing between two joists. Thicker or extra layers of subfloor help the second kind. Only framing work fixes the first kind.
Warning: Sistering joists, adding beams or cutting framing is structural work. If a floor fails a stiffness check, report it. The fix comes from a framer working to the code and, where needed, an engineer, not from the tile crew.
Subfloor Minimums
The Tile Council of North America (TCNA) Handbook method for cement backer board over a wood floor starts with at least 19/32-inch (5/8-inch) exterior-glue tongue-and-groove plywood on joists 16 inches on center. Some backer board and membrane makers allow 23/32-inch OSB, and their instructions say so. Natural stone methods typically call for a second layer of plywood. Check the exact method you are following, since it sets the subfloor, the joist spacing and the layers above.
Before you build on the subfloor:
- Screw down any loose panels into the joists.
- Replace soft, swollen or delaminated panels.
- Check that panel edges are supported or tongue-and-groove.
- Leave about 1/8 inch between plywood panels, the gap panel makers call for, so they can swell without peaking.
Concrete Slabs
A slab is usually stiff enough. Its problems are bond, moisture and cracks.
The Water Drop Test
Sprinkle a few drops of water on the slab in several spots. If the water soaks in and darkens the concrete within a minute or so, the surface is open enough for mortar to grip. If it beads up, something is sealing the surface: a curing compound, sealer, paint or old adhesive. Remove it by grinding or shotblasting with dust controls before you go on.
Warning: Old black adhesive and old resilient flooring residue may contain asbestos. Do not grind, sand or scrape it until it has been tested.
Reading Cracks
| Crack | What it usually means | What to do |
|---|---|---|
| Hairline, flat, not moving | Normal shrinkage | Crack isolation membrane, per the maker |
| Saw-cut control joint | Planned crack location | Follow the method and the membrane maker. Ask before bridging it |
| Expansion or isolation joint | The building moves here | Carry a soft joint up through the tile. Never tile over it solid |
| Wide, growing or one side higher | Structural movement | Stop. An engineer must evaluate it |
A crack isolation membrane is a thin sheet or liquid layer that lets a hairline crack open slightly without cracking the tile above. Look for products that meet ANSI A118.12. Each maker says how far past each side of the crack the membrane must extend, and some want the whole floor covered. Read their sheet.
Moisture testing a slab and correcting flatness are covered elsewhere. Do both before any tile goes down.
Choosing What Goes Over the Subfloor
Tile almost never goes directly on plywood or OSB. Something has to sit between them.
| Layer | What it does | Where it fits |
|---|---|---|
| Cement backer board | Stable, water-tolerant base for mortar | Floors, walls, showers with a membrane |
| Fiber-cement backer board | Similar, lighter, smoother face | Floors and walls per the maker |
| Uncoupling membrane | Lets the subfloor and tile move separately | Floors over wood or concrete, per the maker's subfloor rules |
| Crack isolation membrane | Bridges small cracks | Slabs with hairline cracks |
| Bonded waterproof membrane | Stops water at the tile layer | Showers, wet floors (ANSI A118.10) |
| Glass mat gypsum backer | Water-resistant board for walls | Tub and shower walls, per the maker |
Cement board is not waterproof. Water passes through it without damaging it. In a shower, it needs a liner behind it or a membrane on its face.
Surfaces That Do Not Take Tile Directly
- Particleboard and hardboard underlayment.
- Thin luan and other plywood that is not rated for the method.
- Paper-faced drywall or green board in a tub or shower.
- Plank subfloors without a layer of plywood or another approved layer over them.
- Old vinyl or painted floors, unless the method and mortar maker allow them with special prep.
Installing Backer Board on Floors
- Plan the layout. Stagger the board joints from the subfloor joints, and keep board edges off the subfloor seams.
- Cut it. Score cement board several times with a carbide scoring knife and snap it, or use shears. A circular saw on cement or fiber-cement board makes silica dust, so use a saw with a dust collector and follow your silica plan.
- Bed it. Spread the thin-set the board maker calls for on the subfloor with the notch they name, and set the board into it while it is fresh. This mortar fills voids under the board. It is not glue, and the board still needs every fastener.
- Fasten it. Use the screws or nails the board maker names, at their spacing, with heads set flush. Do not overdrive, which breaks the board's face.
- Gap it. Leave the gaps the maker calls for between boards and at walls.
- Tape the joints. Embed alkali-resistant mesh tape in the same type of mortar you will set tile with.
Installing an Uncoupling Membrane
- Check that the subfloor and joist spacing meet the membrane maker's minimums.
- Mix the mortar the maker names. Many call for unmodified thin-set under and over the membrane. Read the current sheet, since this has changed over the years.
- Comb mortar with the notch they specify, and set the fleece side of the membrane into it.
- Embed it with a float, working from the center to the edges to push out air.
- Lift a corner now and then. The fleece should be fully covered with mortar.
- Butt seams and treat them as the maker says, and leave the perimeter gap they call for.
Keep foot traffic off a freshly bedded membrane, or lay boards to walk on, so it does not shift.
Walls Behind Tile
- Tub and shower walls. Codes such as the International Residential Code list cement, fiber-cement and glass mat gypsum backers for tile in tub and shower areas. Paper-faced gypsum, including green board, does not belong there. Water-resistant gypsum board must not go over a vapor retarder in a shower or tub compartment.
- Dry walls. Sound, flat drywall is a common base for backsplashes and dry walls, with the right mortar or adhesive.
- Flat and plumb. Run a straightedge across the studs before the board goes up. Plane high studs and shim low ones. Board follows the framing, and so will the tile.
Heated Floors
Electric floor-warming mats and cables are embedded in mortar or self-leveling underlayment under the tile. Follow the heating maker's layout and embedment rules exactly. Its instructions call for resistance checks before, during and after the install, so a damaged cable is caught before tile covers it. An electrician makes the electrical connection.
Common Mistakes
| Mistake | What it costs |
|---|---|
| Tiling a bouncy floor | Cracked grout and tile within months |
| Skipping the mortar bed under backer board | Hollow board that flexes and cracks tile |
| Tiling over a slab expansion joint | A crack that comes straight up through the tile |
| Using drywall or green board in a shower | Soft, moldy walls and loose tile |
| Grouting over a membrane seam the maker said to treat | Leaks or cracks at the seam |
| Ignoring a sealed slab | Tiles that pop loose with a hollow sound |
Check Your Understanding
1. Joists span 15 feet. What is the most they can deflect for porcelain tile, and for stone?
180 inches / 360 = 1/2 inch for porcelain. 180 / 720 = 1/4 inch for stone.
2. Water beads up on a slab in three spots. What does that tell you?
Something is sealing the surface, such as a curing compound or sealer. Remove it mechanically, with dust controls, before setting tile.
3. A slab has a crack where one side sits about 1/8 inch higher than the other. Can a crack isolation membrane cover it?
No. An offset crack points to structural movement. Stop and have an engineer evaluate it.
4. A coworker wants to tile a shower over green board to save time. What do you say?
Paper-faced gypsum and green board do not belong in a tub or shower. Use a backer the code and maker allow, with the waterproofing the system calls for.
5. Why do you spread thin-set under backer board if the screws hold it down?
The mortar fills voids between the board and the subfloor, so the board is fully supported and does not flex under the tile.
Key Takeaways
- Check stiffness first. L/360 for ceramic and porcelain, L/720 for stone.
- Report floors that fail. Framing and structural fixes are not tile work.
- Make a slab bondable, and match each crack to the right fix.
- Choose backer board or a membrane for the area, and follow its maker's sheet.
- Keep paper-faced drywall out of showers.
- Carry building expansion joints up through the tile.