Skip to content

Soldering & Brazing Fundamentals

20 min read Training Guide

Understand how solder and brazing filler flow into a joint, then choose the filler and flux, prepare the surfaces, and judge the finished joint.

Table of contents

Soldering and brazing join metal without melting it. You heat the parts until they are hot enough to melt a filler metal, and the filler flows into the gap between them. The same ideas apply to a copper water line, a refrigerant line, a circuit board and a sheet metal seam. Most bad joints trace back to the same few causes, so learning the principles saves you on every job.

What You Will Be Able to Do

  • Tell soldering from brazing and from welding.
  • Explain capillary action and wetting, and why a joint fails without them.
  • Pick a filler family and a flux for the metals you are joining.
  • Prepare a joint in the right order.
  • Look at a finished joint and name what went wrong.

Soldering, Brazing and Welding

The difference comes down to temperature and whether the base metal melts.

Process Filler melts at Base metal melts?
Soldering Below 840 F (450 C) No
Brazing Above 840 F (450 C) No
Welding Near the base metal's melting point Yes

Brazed joints are usually much stronger than soldered joints and can handle higher temperatures. Soldered joints need less heat, so they are gentler on nearby parts.

Neither process makes a joint that is safe above the temperature where the filler softens. If a part runs near that temperature in service, the filler can remelt and the joint can come apart. Choose a filler that melts well above the highest temperature the joint will ever see.

How the Filler Gets Into the Joint

Two things make these joints work.

Capillary action is the force that pulls a liquid into a narrow gap. It is why a paper towel soaks up a spill. In a joint, surface tension draws molten filler into the tight space between the parts, even uphill. You feed filler at one point and it travels through the whole joint on its own.

Wetting is how well molten filler spreads across and bonds to the base metal. Water beads up on a waxed car and spreads out on clean glass. Filler acts the same way. On clean, hot, oxide-free metal it spreads into a thin film. On dirty or cold metal it forms balls and rolls off.

Capillary action only works if the gap is right.

Joint Typical clearance
Soldering 0.002 to 0.005 inch
Brazing 0.001 to 0.005 inch

If the gap is too tight, filler cannot get in. If it is too wide, capillary force is too weak to hold the filler, so it leaves voids or runs out. Factory copper fittings are made with the right clearance for the matching tube. On parts you make yourself, you have to design it in. Remember that metal grows when hot, so two different metals can change the gap at brazing temperature.

What Flux Does

Hot metal reacts with oxygen and grows an oxide skin almost instantly. Filler will not wet oxide. Flux does two jobs: it removes the oxides on the surface, and it blankets the joint so new oxides cannot form while you heat it. Flux does not clean off dirt, oil or heavy tarnish. That is your job before it goes on.

Flux type Used for Residue
Rosin Electronics Non-corrosive, non-conductive
No-clean Electronics production Minimal, usually left on
Water-soluble organic acid Electronics, some plumbing Corrosive, wash it off
Zinc chloride acid flux Sheet metal, general metalwork Corrosive, wash it off
Plumbing paste flux Copper water tube Mildly corrosive, wipe it off
Borax or fluoride brazing flux Brazing Corrosive, remove with hot water

Warning: Never use acid flux on electronics. The residue conducts electricity and eats traces and leads over time.

Match the flux's working temperature to the filler. A soldering flux burns away long before brazing temperature. Brazing flux is often a white paste that turns clear and glassy when the joint reaches temperature, which gives you a built-in thermometer.

Choosing a Filler

Solders

Alloy Melts at about Common use
63/37 tin-lead 361 F Electronics where lead is still allowed
SAC305 (tin, 3% silver, 0.5% copper) 422 F Lead-free electronics
Tin-copper (99.3/0.7) 441 F Lead-free plumbing and electronics
Tin-antimony (95/5) 452 F Lead-free plumbing, higher strength
Tin-silver (96/4) 430 F Lead-free plumbing and specialty work

Lead is a cumulative toxin, meaning it builds up in the body, and it leaches from solder into drinking water. For that reason, 50/50 tin-lead solder has been illegal on drinking water systems in the United States since the 1986 Safe Drinking Water Act amendments. Today, solder and flux used on drinking water systems can contain no more than 0.2 percent lead. Many electronics are also limited to lead-free solder by rules such as the European RoHS directive, though some aerospace, military and medical work still uses tin-lead.

Solder comes as wire (solid or with a flux core), bar, paste for surface-mount boards, and preformed shapes for production work.

Brazing Filler Metals

Family What it joins Flux needed?
BCuP (copper-phosphorus) Copper to copper No, it fluxes itself on copper
BCuP (copper-phosphorus) Copper to brass or bronze Yes
BAg (silver) Steel, stainless, copper, brass, mixed metals Yes
BCu or RBCuZn (copper, brass) Steel and cast iron, at higher heat Yes

The phosphorus in BCuP removes copper oxide, which is why it needs no flux on copper. It does not work that way on other metals. On steel, stainless steel or nickel alloys, the phosphorus forms brittle compounds, so do not use BCuP there. Switch to a BAg filler with flux.

Heat Sources

Heat source Good for
Soldering iron Electronics, small wires
Propane or MAP-type torch Soldering copper tube
Air-acetylene torch Soldering, brazing smaller tube
Oxy-acetylene torch Brazing larger tube, steel and heavy parts
Induction or furnace High-volume production brazing

An oxy-acetylene flame reaches about 5,700 F, far hotter than brazing needs, so control comes from how you move the flame and not from the flame temperature. Air-fuel torches run cooler and give you more time.

Preparing Any Joint

Every sound joint follows the same order. Skip a step and the joint will tell you later.

  1. Cut square so the parts seat fully.
  2. Deburr the edges. Burrs block seating and restrict flow in tube.
  3. Clean to bright metal with abrasive cloth, a fitting brush or a nylon pad. Remove oil with a suitable solvent.
  4. Flux both surfaces with a thin, even coat, if the filler needs flux.
  5. Assemble right away and support the parts so they cannot move.
  6. Heat the joint, starting with the heavier part. The metal melts the filler, not the flame.
  7. Feed filler at the joint and let capillary action draw it in.
  8. Let it cool undisturbed. Do not quench it. Movement or thermal shock while it freezes can crack it.
  9. Clean off flux residue as the flux type requires.

Do not touch cleaned surfaces with bare fingers, because skin oil blocks wetting. Clean shortly before you assemble, because bright metal begins to tarnish again.

Worked Example: A 3/4 Inch Copper Water Joint

This is the sequence in ASTM B828, the standard practice for making capillary joints by soldering copper tube and fittings. Local plumbing codes and your employer's procedure still apply.

  1. Cut the tube square and ream the inside burr.
  2. Mechanically clean the tube end and the fitting socket to bright copper.
  3. Brush on a thin coat of lead-free flux and push the tube fully into the socket with a slight twist.
  4. Heat the fitting, moving the flame around it. Keep the flame off the solder.
  5. Touch solder to the joint on the side away from the flame. If it melts on contact, the joint is ready.
  6. Feed solder until a full ring shows at the joint. A useful rule says the length of solder you need is about equal to the tube diameter, so about 3/4 inch of wire here.
  7. Wipe the joint while it is still hot, then let it cool without moving it.

Too much flux or solder does not help. Extra solder can run inside the tube, and leftover flux keeps attacking the copper.

Judging a Finished Joint

A good joint shows a smooth, continuous fillet of filler all the way around, with no gaps, voids or pinholes. The filler should blend into the base metal at a shallow angle, which shows it wetted the surface.

What you see Likely cause Fix
Filler balls up and will not flow Dirty or oxidized metal, or metal too cold Clean again, reflux, heat the base metal
Filler runs out of the gap Gap too wide Refit the joint or use a closer fit
Filler stops partway in Uneven heat or gap too tight Heat the whole joint evenly
Porous or spongy joint Moisture, burned flux or dirty filler Dry the joint, reflux, use fresh filler
Flux trapped in the joint Too little heat or too wide a gap Heat evenly and feed filler to push flux out
Black, burned flux Overheating Reclean and redo with less heat
Dull, grainy solder Joint moved while cooling Reheat, reflow and hold still
Crack after cooling Movement, quenching or too much stress Support the joint and let it cool naturally

Overheating does real damage. Flux burns off and stops protecting the joint, heavy oxide forms, and hot filler can eat into thin base metal. More heat is not a fix for a dirty joint.

Most failed joints come down to two causes: the joint is not hot enough, or it is not clean enough. Check both before you change anything else.

Staying Safe

Torch work is hot work, so fire precautions and any permit your site requires apply before you light up. A few hazards are specific to joining metals:

  • Fumes. Work with local exhaust or good ventilation, and keep your face out of the smoke. Rosin flux fume can cause occupational asthma, and brazing fluxes can release fluorides.
  • Cadmium. Some older silver brazing alloys contain cadmium, and the fume can kill. Use cadmium-free fillers. Check the Safety Data Sheet before you heat an unknown rod.
  • Lead. Wash your hands before you eat, drink or smoke, and keep food out of the work area.
  • Burns. Copper and steel stay hot long after they stop looking hot. Wear eye protection, because flux and molten solder can pop.

Warning: Never heat a closed or pressurized system. Trapped liquid or gas expands and can rupture the line, and drained lines can still hold water, fuel or refrigerant. Make sure the system is open and verified empty by someone qualified to do it.

Common Mistakes

  • Heating the filler and not the joint. The filler melts but never bonds. The joint leaks.
  • Skipping the cleaning because the metal looks fine. Invisible oxide costs you a rework.
  • Using lots of flux to make up for poor cleaning. Flux cannot replace abrasive cleaning.
  • Using BCuP on steel. The joint turns brittle and can fail in service.
  • Quenching a hot joint to save time. Thermal shock can crack the joint.

Check Your Understanding

A coworker heats a copper fitting and the solder melts, but it sits in a ball on the tube. What are the two most likely problems?

The metal is not clean, the joint is not hot enough, or both. Solder that beads is not wetting, so reclean, reflux and heat the base metal, not the solder.

You need to join a copper tube to a steel fitting. Which filler family do you reach for?

A silver (BAg) filler with flux. Copper-phosphorus filler is only self-fluxing on copper and turns brittle on steel.

A brazed part will run at 900 F in service. Is a tin-silver solder a sensible filler?

No. That solder melts near 430 F, so the joint would come apart. Use a brazing filler that melts well above the service temperature.

Why can't a wide, sloppy gap be fixed by feeding in more filler?

Capillary force gets weaker as the gap widens. The filler will not stay in the gap, and you end up with voids and a weak joint.

Key Takeaways

  • Soldering is below 840 F and brazing is above it. In both, the base metal stays solid.
  • Capillary action and wetting do the work. They need the right gap, clean metal and even heat.
  • Flux removes and blocks oxides, but it does not replace cleaning.
  • Match the filler and flux to the metals and the service temperature. Use lead-free solder on drinking water systems.
  • Heat the joint, not the filler, and let it cool on its own.
  • If filler will not flow, the joint is too cold, too dirty, or both.